JEOS RP ISSN02 | Page 198

J. Eur. Opt. Society-Rapid Publ. 21, 50( 2025) 193
Table 1. Grating substrate parameters determined from EMA and RCWA models. AFM values from previous work [ 13 ] are also reported for comparison.
EMA model
RCWA model
AFM results
EMA layer thickness( T)
22 nm
Grating depth( d)
22 nm
22 nm
EMA layer density( q)
0.835 g / cm 3
Grating FWHM( ff)
0.38
0.51
Grating slope( a)
47 °
47 °
Fig. 7. GIXR measurements for( a, b) N = 6,( c) N = 16 and( d) aperiodic multilayers on gratings in classical mounting. RCWA model of the multilayer grating and IMD simulation of the multilayer on a flat SiO 2 substrate are also plotted in each case.( b) is a close view of the total reflection plateau of( a) and shows an IMD simulation of the multilayer on a flat SiO 2 substrate with a top EMA layer to account for the surface profile.
Table 2. ML grating parameters used in the RCWA models plotted in Figure 7.
N = 6
N = 16
Aperiodic
Grating depth( d)
21.8
22.5
21.2
Grating FWHM( ff)
0.49
0.39
0.48
Grating slope( a)
49 °
41 °
43 °
Top SiO 2 thickness( nm)
1.7
1.7
1.7
DW factor( nm)
0.8
0.8
0.8
same wavelength. For the periodic case for example, at k = 18 nm, the + 1 order presents an experimental peak efficiency of ~ 18 % while the �1 order is about 10 times lower. This effect is due to the fact the efficiency of ML gratings is based on volume diffraction( as opposed to surface diffraction) and that the + 1 and �1 diffracted orders don’ t have the same exit angle inside the ML. Therefore, the Bragg conditions for the ML cannot be satisfied at the same wavelength for both orders [ 31 ]. For the periodic ML grating( Fig. 8a), we can see that the model fits very well with the 0-order efficiency spectrum. The fit of the 0 order is not as good for the aperiodic ML grating( Fig. 8b) andthis may be due to the defects revealed by TEM analyses on the 1st deposited period of the aperiodic ML. For both samples however, there is a large discrepancy between the RCWA model and the experimental data for the �1 order, the- measured peak efficiency being ~ 30 % lower( relative) than the modeled ones.
The DW factor was not included in the RCWA simulations in Figure 8. According to the average roughness previously determined on these ML gratings( about 0.45 nm), we can expect peak efficiencies to be lower by about 5 %( relative) [ 15 ]. This may explain the difference between experimental and simulated data for the + 1-diffraction order, but it will not improve significantly the discrepancy for the �1-diffraction order.
In order to better understand this discrepancy between experimental and simulated efficiencies in the �1-diffraction order, we measured the efficiency of the 6-period ML grating in conical mounting. The results are plotted on Figure 9 for the �1, 0 and + 1 diffraction orders. As for the classical mounting, we observe a much lower peak efficiency in the �1 order than in the + 1 order, while