JEOS RP ISSN02 | Page 210

J. Eur. Opt. Society-Rapid Publ. 21, 52( 2025) 205
Figure 1. Simplified model of the ICP reactor and EEC used to model the sheath region.
Table 1. Etching rate under different plasma parameters.
Gas mixture
Gas flow( sccm)
Etching parameters
Etching rate( nm / min)
Pressure
RF Power
DC Bias
ICP Power
h = 2mm
h = 5mm
h = 10mm
( Pa)
( W)
( V)
( W)
CHF3 / Ar / O 2
50 / 30 / 10
0.5
500
250
100
29.4
32.67
28
205
300
74.6
65.8
41.7
205
500
118
88.7
11.1
160
1000
125
15
0
r = 20 mm. Etching was done in a CHF3 / Ar / O 2 inductively coupled plasma( ICP) discharge using SI 500( PTSA 400 ICP) from SENTECH Instruments GmbH, Berlin. A schematic of the etching chamber is shown in Figure 1a. A current applied to a spiral coil generates a time-varying magnetic field, which in turn induces the electric field that sustains plasma. The inductive source power( ICP power) controls plasma density, while the substrate electrode power( RF power) independently controls sample biasing [ 20, 21 ].
The discharge conditions – gas composition, pressure, RF power, DC bias, and ICP power – are summarized in Table 1. Before the etching, samples were patterned with grating lines by laser interference lithography in the photoresist( Az Ò MIR 701, Microchemicals GmbH). Etching was performed for 2 min. Final etching depths were measured with an atomic-force microscope( AFM)( Dimension 3100d, Veeco).
Figure 2 shows the etching rates as a function of the ICP powerforalletchedsamples. The2mmsampleexhibitsa steady increase in etching rate with increasing ICP power. At 1000 W ICP power, DC bias drops( Table 1), which leads to the saturation of the etching rate. In contrast, samples with thickness 5 and 10 mm show a different trend. Etching rates increase to the maximum at ICP power values 500 W and 300 W, respectively, and then decline at higher power levels.
For the h = 10 mm sample, the etching completely stops at 1 kW ICP power. EDS analysis on this sample showed an elevated presence of carbon together with a high fluorine
content( 20 %), suggesting the presence of a C x F y film deposited on the sample. Oehrlein et al. [ 22 ] reported that during SiO 2 etching, surface passivation by CF x radicals dominates the process below a threshold value of the voltage bias.
In the next chapters, we show that the thickness of a dielectric sample directly affects the sheath potential and, consequently, the ion energy at the surface. If the sample is too thick, it behaves like a floating surface due to the sample’ s low capacitance. This results in suppressed etching because of the insufficient ion energy.
3 Simulations
We simulate a one-dimensional plasma-sheath region spanning from the sample to the sheath-plasma boundary. We adopt a fluid model combined with an Equivalent Electric Circuit model( EEC) and take plasma bulk parameters from the device’ s datasheet. In this chapter, we provide the model description and governing equations.
3.1 Fluid model
We consider a low-pressure, non-magnetized, charge neutral plasma in contact with an RF-biased electrode in the presence of a dielectric substrate. A positively charged plasma sheath region with thickness s is formed between the plasma and the substrate. The following assumptions are made to simplify the model: